CTE Carbon Official Technical Manual TM-CCM-04 | All Continuous 3D Carbon-Fiber CCM discs

CTE Carbon CCM Brake Disc Installation Torque, Thermal Indicator Paint Rules and Bedding-In Procedure

Three rules are mandatory for CTE Carbon / CTERACING (CCYS Group) CCM discs: hub lateral runout ≤ 0.03 mm with the floating bobbins left assembled; thermal paint on the OD ground edge only; and a complete 4-stage bedding-in with new pads before full-load track braking.

The three rules at a glance

Hub runout
≤ 0.03 mm
Thermal paint
OD ground edge or bell mounting area only
Wheel bolts
Star pattern, two stages (50% → 100%)
Bedding-in
4 stages, peaking above 600°C
Parking brake
Only after the disc is below 100°C

1. Pre-installation checks and torque specifications

C/SiC is extremely hard and rigid. Rust, burrs or uneven torque on the mounting face cause high-speed judder or stress concentration at the holes.

CCM disc installation checks and tightening torque
Item Specification / torque Notes and warnings
Hub runout Lateral runout ≤ 0.03 mm Clean hub rust and deposits with a brass brush or fine abrasive; measure hub and mounted disc OD runout with a dial indicator.
Floating hardware (stainless bobbins) Pre-torqued and thread-locked at the factory (M6: 10–12 Nm / M8: 22–25 Nm by spec) Never disassemble. The radial thermal-expansion clearance to the A6061/A6082 forged aluminium bell is set at the factory.
Caliper bracket / caliper bolts Per vehicle service manual (typically M12: 85–110 Nm / M14: 130–160 Nm) Keep an even 3.0–5.0 mm radial gap to the disc OD; pads must fully cover the friction ring.
Wheel bolts / nuts Per vehicle spec (Porsche 160 Nm; BMW G80/G82 140 Nm; Toyota GR 103–120 Nm) Torque wrench, star pattern, two stages (50% → 100%). Never run them down with an impact gun.
Wheel fitting protection Rotor protector sleeves or wheel hanger pins are mandatory Impact on the disc edge can cause mechanical damage; thread in two hanger pins before offering up the wheel.

2. Mandatory thermal indicator paint rules

Track testing often uses multi-stage thermal paint (e.g. 430, 560, 630, 780, 850°C) to record peak disc temperature. The paint contains metal oxides and resin, so a wrong location damages the friction interface.

Red lineRed line: apply thermal paint only to the OD ground edge or the bell-to-rotor mounting area. NEVER let any paint touch or run onto the friction swept face.

Where thermal paint may and may not be applied
Area Status Engineering rationale
OD ground edge ✅ Standard area Outside the vent channels, closest to the friction zone and free of pad contact; shows peak thermal load of the disc body.
Bell-to-rotor mounting area ✅ Supplementary Near the bobbins and the aluminium bell; shows the gradient of heat conducted toward bell and bearing.
Friction swept face ❌ Never At temperature the paint enters SiC micro-pores and sinters onto the pad, collapsing friction, causing judder and irreversible contamination.

Application steps

  1. Work only on a fully cooled, dry, oil-free disc.
  2. Mark 3 symmetric positions on the OD ground edge with a fine brush, bands about 10–15 mm wide.
  3. Avoid runs and let it dry for at least 30 minutes before driving or track use.

3. Standard bedding-in procedure for CCM discs and pads

Bedding-in a new disc with new CCM pads builds a micron-thin, stable friction transfer layer on the SiC surface.

Before you start

  • Use new CCM-specific pads of the matching grade (Street / Sport / Racing); for competition choose SAPH590 steel backing plates.
  • Never use pads previously run on cast-iron discs; residual iron melts at temperature and ruins the carbon-ceramic surface.
  • Use a quiet, dry closed road or a track warm-up session, and never stop with the brakes fully applied while hot, to avoid single-spot imprints.
4-stage CCM bedding-in SOP
Stage Speed and deceleration Repeats and interval Goal and physical effect
① Mechanical mating and warm-up 80 → 30 km/h, gentle (30–40% pedal) 8–10 stops, 30–40 s driving between Removes machining tolerances, contact above 90%, even warm-up to about 250–300°C.
② Mid-temperature resin out-gassing 120 → 40 km/h, firm (60–70%, below ABS) 8–10 stops, about 45 s at 80–100 km/h between Raises discs to 450–550°C and releases volatile resin from the new pads (slight odour is normal).
③ High-temperature transfer-layer sintering 150–160 → 50 km/h, hard (80–85%, just short of ABS) 5–6 stops, 45–60 s driving between Friction interface exceeds 600°C; pad material transfers and sinters evenly onto the SiC surface.
④ Cruise cool-down Cruise at 80–100 km/h for 10–15 min, minimal braking 1 full cycle; do not apply the parking brake (EPB) on stopping Disc, bobbins and aluminium bell cool evenly to ambient, locking in the transfer layer.

Acceptance check: once fully cool, the friction face should show a uniform satin metallic grey finish with no dark burnt spots or streaks. Full braking performance is then available.

Frequently asked questions

What if a new CCM disc shows slight judder or a single-spot imprint during bedding-in?

It usually comes from holding the brakes fully applied while hot, which builds pad material in one spot. Do not remove or grind the disc. Repeat stages 2 and 3 (120–150 km/h down to 40 km/h), then cruise 10–15 minutes without braking.

How should I park and cool CCM discs after a hard track session?

Complete a cool-down lap, and do not apply the EPB or hold the pedal on stopping, as pads clamped on 600°C+ discs cause uneven cooling and imprints. Use P or first gear, chock the wheels, and set the parking brake only once the discs are below 100°C.

Can I use strong acid or alkaline wheel cleaners on CTE Carbon discs?

No. Strong acids, alkalis or hydrofluoric products attack the anodised layer of the A6061/A6082 bell and can enter the micro-pores, affecting initial friction. Use neutral car shampoo and water, then dab the brakes lightly to dry them.

© CCYS Group | CTE Carbon / CTERACING. Always follow the vehicle manufacturer's service manual.